Tool Steels
Tool and Die Steel Includes Cold Work Steel, Hot Work Steel, Plastic Mould Steel, High Speed Steel. These tool materials adhere to great quality demands of steel like temper, strength, toughness, resistance to tempering, hardening capacity, dimensional stability etc. The range of Tool Steel in our store includes products from renowned manufacturers.
Main characteristics and applications
Cutting tools for sheets up to 4 mm thickness, trimming dies, blanking dies for paper and plastics, shear blades and rotary shear blades for sheet thicknesses up to 2 mm, drawing and deep-drawing tools. Woodworking tools, stone pressing tools, pressure pads and highly wear-resistant plastic moulds, profile rolls.
Steel properties
12 % ledeburitic chromium tool steel with extreme wear resistance.
Comparable standards
DIN | W.Nr | AISI/ASIM |
---|---|---|
X210Cr12 | 1.2080 | D-3 |
Chemical composition (typical; in weight %)
C | Si | Mn | P(Max) | S(Max) | Cr |
---|---|---|---|---|---|
1.90-2.20 | 0.10-0.60 | 0.20-0.60 | 0.03 | 0.03 | 11.0-13.0 |
Physical properties (reference values)
20°C | 100°C | 250°C | 500°C | |
---|---|---|---|---|
Coefficient of thermal expansion at °C 10-6 m/(W/mk) | 10.8 | 11.7 | 12.2 | 12.8 |
Thermal conductivity at °C (W/mk) | 16.7 | - | - | - |
Heat treatment
TREATMENT | TEMPERATURE | HOLDING TIME (HT) | COOLING | COMMENTS |
---|---|---|---|---|
Annealing | Heat to 800 – 840 °C | Min. H.T. for 2 minute /mm | Furnace | HARDNESS : max. 250 |
Stress relieving | Heat to 650 – 700 °C | Min. H.T. for 2 minute /mm | furnace | - |
Hardening | Heat to 930 – 960 and 950 - 980 °C | Min. H.T. for 1 minute /mm | - | HARDNESS : 64 |
Note
°C | 100 | 200 | 300 | 400 | 500 | 600 |
---|---|---|---|---|---|---|
HRC | 63 | 62 | 59 | 57 | 54 | 46 |